How the quantities are worked out
A mix design states how much of each material goes into one cubic metre of compacted concrete. To batch any other volume, every figure is multiplied by the same factor: the volume you need, plus an allowance for waste. Cement is then divided by the bag size and rounded up, because part bags are not sold.
Order volume V = volume × (1 + waste % ÷ 100)
Quantity of each material = amount per m³ × V
Cement bags = cement in kg ÷ bag size in kg, rounded up
The grade name follows the strength classes of EN 206. In C30/37, 30 MPa is the characteristic strength of a standard cylinder and 37 MPa that of a 150 mm cube, both at 28 days. The target mean strength in the table is the characteristic strength plus 8 MPa, the relationship Eurocode 2 (EN 1992-1-1) uses between the two. The water-to-binder ratio is free water divided by cement, and the mass ratio is cement : sand : coarse aggregate with cement set to 1.
Quantities per cubic metre
| Per m³ | C20 | C25 | C30 | C35 | C40 | C45 |
|---|---|---|---|---|---|---|
| Cylinder / cube strength | 20/25 MPa | 25/30 MPa | 30/37 MPa | 35/45 MPa | 40/50 MPa | 45/55 MPa |
| Target mean strength | 28 MPa | 33 MPa | 38 MPa | 43 MPa | 48 MPa | 53 MPa |
| Water-to-binder ratio | 0.58 | 0.52 | 0.46 | 0.42 | 0.38 | 0.34 |
| Mass ratio C : FA : CA | 1 : 2.48 : 3.63 | 1 : 2.14 : 3.26 | 1 : 1.87 : 2.99 | 1 : 1.65 : 2.76 | 1 : 1.52 : 2.57 | 1 : 1.35 : 2.41 |
| Cement | 310 kg | 345 kg | 380 kg | 415 kg | 445 kg | 480 kg |
| Cement in 50 kg bags | 6.2 | 6.9 | 7.6 | 8.3 | 8.9 | 9.6 |
| Free water | 180 L | 180 L | 175 L | 174 L | 169 L | 163 L |
| Sand (fine aggregate) | 770 kg | 740 kg | 710 kg | 685 kg | 675 kg | 650 kg |
| Coarse aggregate 10–20 mm | 1,125 kg | 1,125 kg | 1,135 kg | 1,145 kg | 1,145 kg | 1,155 kg |
| Chemical admixture | 0–1.5 L | 1.4–2.1 L | 2.3–3.0 L | 3.3–4.2 L | 4.5–5.8 L | 5.8–7.7 L |
| Fresh wet density | ≈2,385 kg | ≈2,392 kg | ≈2,403 kg | ≈2,423 kg | ≈2,439 kg | ≈2,455 kg |
Each column checks itself. For C30, 175 ÷ 380 = 0.46 is the water-to-binder ratio, 710 ÷ 380 = 1.87 and 1,135 ÷ 380 = 2.99 give the mass ratio, and 380 + 175 + 710 + 1,135 = 2,400 kg, which with the admixture is close to the 2,403 kg density. Moving up the grades, cement rises and water falls, so the ratio drops and the strength climbs. That is the main lever of every mix design.
Worked example: 3 m³ of C30
A footing needs 3 cubic metres of C30 concrete, and you allow 5% for waste.
- Order volume. 3 × 1.05 = 3.15 m³.
- Cement. 380 × 3.15 = 1,197 kg. In 50 kg bags that is 1,197 ÷ 50 = 23.94, so 24 bags.
- Free water. 175 × 3.15 = 551.25 litres.
- Sand. 710 × 3.15 = 2,236.5 kg.
- Coarse aggregate. 1,135 × 3.15 = 3,575.25 kg.
- Admixture. 2.3 × 3.15 = 7.245 litres up to 3.0 × 3.15 = 9.45 litres, at the dose the product data sheet gives.
Getting a good batch
Correct the water for wet sand. The table assumes aggregate that is saturated but surface-dry. Sand from a stockpile usually carries extra water. If C30 sand holds 4% surface moisture, 710 × 0.04 = 28.4 kg of water arrives with it, so weigh out 710 + 28.4 = 738.4 kg of wet sand and add 175 − 28.4 = 146.6 litres of water. Skipping this step raises the real water-to-binder ratio and costs strength.
Batch by mass, not by shovel. The quantities are masses. Sand bulks when damp, so a bucket of it holds a different mass from one day to the next. If you must batch by volume, ask your supplier for the bulk density of their material and convert.
Do not add water to make it flow. The admixture range is there to give workability without extra water. Follow the dose on the product data sheet rather than the midpoint of the range.
Know where the table stops. These are typical proportions for ordinary cement and 10–20 mm aggregate. Exposure class, cement type, aggregate shape and the slump required all change a real design. For structural work, the grade comes from the engineer's specification, and the mix from a supplier or a trial batch tested against the relevant standard, such as AS 1379 in Australia or EN 206 in Europe.